In this study, hard wear-resistant Ti-Si-C coatings were deposited on Cu-Cr materials to improve their performance as sliding electrical contact materials. A ceramic disk composed of Ti3SiC2 and TiC phases was used as a target for DC magnetron sputtering to deposit the coatings. The influence of the power supplied to the magnetron on the chemical composition, structure, and friction coefficient of the coatings was examined. The coatings demonstrated high hardness (23-25 GPa), low wear rate (1-3 × 10-5 mm3/N/m) and electrical resistance (300 µOhm·cm), and fair resistance to electroerosion. The coating deposited at 450 W for 30 min displayed optimal properties for protecting the Cu-Cr alloy from the arc effect.