Assessment of physical properties of bioactive glass-modified universal multimode adhesive and its bonding potential to artificially induced caries affected dentin.
Kazem, Nada E; El-Refai, Dina A; Alian, Ghada.
Afiliação
  • Kazem NE; Dental Biomaterials Department, Faculty of Dentistry, Ain Shams University, African Union Organization Street, Abbasia, Cairo, 11566, Egypt. Nada.Kazem@asfd.asu.edu.eg.
  • El-Refai DA; Dental Biomaterials Department, Faculty of Dentistry, Ain Shams University, African Union Organization Street, Abbasia, Cairo, 11566, Egypt.
  • Alian G; Dental Biomaterials Department, Faculty of Dentistry, Ain Shams University, African Union Organization Street, Abbasia, Cairo, 11566, Egypt.
BMC Oral Health ; 24(1): 423, 2024 Apr 05.
Article em En | MEDLINE | ID: mdl-38580948
ABSTRACT

BACKGROUND:

To evaluate the physical properties of bioactive glass-modified universal multimode adhesive and its micro-tensile bond strength (µTBS) to artificially induced caries-affected dentin.

METHODS:

All bond universal adhesive was used in the study. Specimens were divided into 2 main groups control unmodified adhesive and 5 wt% BAG modified adhesive. The degree of conversion, pH, bioactivity, and viscosity of the adhesives were tested with n = 5 for each test. Micro-tensile bond strength evaluation was done in etch & rinse (ER) and selective-etch (SE) modes, where 24 human molar teeth were used (n = 3), 12 teeth for immediate bond strength, and the other 12 were tested after 6 months of storage in simulated body fluid (SBF).

RESULTS:

No significant difference was found between the control and the 5wt% BAG groups regarding the degree of conversion (61.01 ± 0.43 and 60.44 ± 0.61 respectively) and the viscosity (109.77 ± 22.3 and 124.3 ± 9.92 respectively). The control group revealed significantly lower pH values than the 5wt% BAG group (3.16 ± 0.5 and 4.26 ± 0.09 respectively). Immediate bond strength results revealed that the 5wt% BAG in the ER mode had the highest bond strength followed by the control group in the ER mode (44.16 ± 7.53 and 44.00 ± 7.96 respectively). SE groups showed that the immediate strength of the 5wt% BAG group was higher than the control group (42.09 ± 6.02 and 39.29 ± 6.64 respectively). After 6 months of storage, bond strength results revealed a decrease in bond strength values for the control groups but not for the 5wt% BAG in both application modes.

CONCLUSIONS:

The incorporation of BAG (5wt%) improved the universal adhesive micro-tensile bond strength and bond durability for both adhesive application modes without affecting its degree of conversion or viscosity.
Assuntos
Palavras-chave

Texto completo: 1 Coleções: 01-internacional Base de dados: MEDLINE Assunto principal: Colagem Dentária / Cárie Dentária Limite: Humans Idioma: En Revista: BMC Oral Health Ano de publicação: 2024 Tipo de documento: Article

Texto completo: 1 Coleções: 01-internacional Base de dados: MEDLINE Assunto principal: Colagem Dentária / Cárie Dentária Limite: Humans Idioma: En Revista: BMC Oral Health Ano de publicação: 2024 Tipo de documento: Article