Effects of different polishing techniques on the surface roughness of dental porcelains
Sarikaya, ISil; Güler, Ahmet Umut.
Afiliación
  • Sarikaya, ISil; Ondokuz Mayis University. Faculty of Dentistry. Department of Prosthodontics. Samsun. TR
  • Güler, Ahmet Umut; Ondokuz Mayis University. Faculty of Dentistry. Department of Prosthodontics. Samsun. TR
J. appl. oral sci ; J. appl. oral sci;18(1): 10-16, Jan.-Feb. 2010. ilus, tab
Article en En | LILACS | ID: lil-545021
Biblioteca responsable: BR1.1
ABSTRACT

OBJECTIVE:

The purpose of this study was to evaluate the effects of different polishing techniques on the surface roughness of dental porcelains. MATERIAL AND

METHODS:

Fifty-five cylindirical specimens (15x2 mm) were prepared for each feldspathic (Vita VMK 95, Ceramco III) and low-fusing dental porcelain (Matchmaker). Fifty-five specimens of machinable feldspathic porcelain blocks (Vitablocs Mark II), (12x14x18 mm) were cut into 2-mm-thick slices (12x14 mm) with low speed saw. The prepared specimens were divided into 11 groups (n=5) representing different polishing techniques including control ((C) no surface treatment), glaze (G) and other 9 groups that were finished and polished with polishing discs (Sof-Lex) (Sl), two porcelain polishing kits (NTI (Pk), Dialite II (Di)), a diamond polishing paste (Sparkle) (Sp), a zirconium silicate based cleaning and polishing prophy paste (Zircate) (Zr), an aluminum oxide polishing paste (Prisma Gloss) (Pg), and combinations of them. The surface roughness of all groups was measured with a profilometer. The data were analyzed with a 2-way analysis of variance, and the mean values were compared by the Tukey Honestly Significant Difference test (a=0.05).

RESULTS:

For all porcelain material groups, the lowest Ra values were observed in Group Gl, Group Sl, Group Pk, and Group Di, which were not significantly different from each other (p>0.05).When comparing the 4 different porcelain materials, the machinable feldspathic porcelain block group (Mark II) demonstrated statistically significantly less Ra values than the other porcelain materials tested (p<0.05). No significant difference was observed between the VMK 95 and Ceramco III porcelain groups (p=0.919), also these groups demonstrated the highest Ra values.

CONCLUSION:

Subjected to surface roughness, the surfaces obtained with polishing and/or cleaning-prophy paste materials used alone were rougher compared to the surfaces finished using Sof-lex, Dialite, ...
Asunto(s)
Palabras clave
Texto completo: 1 Bases de datos: LILACS Asunto principal: Pulido Dental / Porcelana Dental Tipo de estudio: Clinical_trials Límite: Humans Idioma: En Revista: J Appl Oral Sci / J. appl. oral sci / J. appl. oral sci. (Online) / Journal of applied oral science (Impresso) Asunto de la revista: ODONTOLOGIA Año: 2010 Tipo del documento: Article País de afiliación: Turquía
Texto completo: 1 Bases de datos: LILACS Asunto principal: Pulido Dental / Porcelana Dental Tipo de estudio: Clinical_trials Límite: Humans Idioma: En Revista: J Appl Oral Sci / J. appl. oral sci / J. appl. oral sci. (Online) / Journal of applied oral science (Impresso) Asunto de la revista: ODONTOLOGIA Año: 2010 Tipo del documento: Article País de afiliación: Turquía