RESUMO
In order to discuss the anti-Thiobacillus corrosion performance of geopolymer solidification MSWI fly ash, the research simulated the Thiobacillus corrosion process by experiment, investigated the change of mass, compressive strength, leaching concentration. The results showed that geopolymer had a good anti-corrosion ability: weight loss within 1%, the compressive strength still reached 21.88 MPa after 28 days, the corrosion resistance coefficient was above 0.9. The maximum leaching concentration of Cr, Cu, Zn, Cd, Hg, Pb were 107.7 microg x L(-1), 22.71 microg x L(-1), 39.18 microg x L(-1), 0.56 microg x L(-1), 34.84 microg x L(-1) and 3.03 microg x L(-1), respectively. And the leaching concentration of geopolymer reduced with the immersion time, showed a good anti-Thiobacillus corrosion performance. Through the X-ray diffraction, Fourier transform infrared spectroscopy, scanning electron microscope spectra of geopolymer, we investigated the microstructure and mechanism of geopolymer anti-corrosion.